Sponge Iron Powder (30,000t)
One:Sponge Iron Powder Process | ||||||||||||||||||
Iron Ore →Roughing→Cleaning→Reduction in Tunnel Kiln→Crushing and Magnetic Separation→Reduction Furnace→Crushing→Screening→Batching→Packaging | ||||||||||||||||||
Two:Standard, Properties and Application of Sponge Iron Powder |
Sponge Iron Powder
Grade | Chemical Composition£¨%£© | Physical Properties | Particle Size% | Properties | Application | |||||||||||
C≤ | Si≤ | Mn≤ | P≤ | S≤ | HL≤ | TFe≥ | Apparent Density g/cm3 | Flowability S/50g | Compressibility g/cm3 | + 100 |
+200-100 | +325-200 | -325 | |||
g≤ | at 5t pressure | |||||||||||||||
JHF 100.23 |
0.015 | 0.010 | 0.010 | 0.009 | 0.009 | 0.30 | 99.00 | 2.20-2.45 | 35 | 6.62 | ≤3 | 36-46 | balance | 18-30 | Low apparent density, high purity, and high formability | Oilless Bearings, low density special-shaped PM parts |
JHF 100.25 |
0.015 | 0.010 | 0.010 | 0.009 | 0.009 | 0.30 | 99.00 | 2.40-2.60 | 32 | 6.65 | ≤3 | 38-48 | balance | 18-30 | High purity, high compressibility, and high formability | Medium-high density PM parts |
JHF 100.27Z |
0.012 | 0.010 | 0.010 | 0.009 | 0.009 | 0.24 | 99.00 | 2.65-2.80 | 32 | 6.74 | ≤3 | 40-50 | balance | 15-25 | High apparent density, high purity, and high compressibility | Medium-high density PM parts |
JHF 100.27C |
0.010 | 0.010 | 0.010 | 0.009 | 0.009 | 0.24 | 99.00 | 2.60-2.80 | 32 | 6.74 | ≤3 | 35-45 | balance | 18-30 | High apparent density, high purity, and high compressibility | Medium-high density PM parts and magnetic materials |
JHF 200.26 |
0.015 | 0.010 | 0.010 | 0.009 | 0.009 | 0.27 | 99.00 | 2.50-2.70 | 36 | 6.70 | 0 | +200 | 30-45 | balance | High purity, high compressibility and high fine powder content | Magnetic materials, friction materials and hard metal |
≤3 | ||||||||||||||||
JHF 200.27 |
0.010 | 0.010 | 0.010 | 0.009 | 0.009 | 0.27 | 99.00 | 2.60-2.80 | 36 | 6.72 | 0 | +200 | 35-45 | balance | High purity, high compressibility and high fine powder content | Magnetic materials, friction materials and hard metal |
≤8 | ||||||||||||||||
JHF 300 |
0.015 | 0.010 | 0.010 | 0.009 | 0.009 | 0.33 | 99.00 | ¡¡ | ¡¡ | 6.60 | ¡¡ | +325 | 400-325 | -400 | High purity, large content of ultrafine powders | Magnetic materials, friction materials and hard metal |
≤5 | 20-40 | balance | ||||||||||||||
JHF 400 |
0.017 | 0.010 | 0.010 | 0.009 | 0.009 | 0.37 | 98.70 | ¡¡ | ¡¡ | 6.55 | ¡¡ | +400 | +500-400 | -500 | ||
≤8 | balance | ≥55 |
Copper Coated Powder
Grade | Chemical Composition£¨%£© | Physical Properties | Particle Size% | Properties | Application | |||||||
Cu | HL≤ | Apparent Density g/cm3 | Flowability S/50g | Compressibility g/cm3 | + 100 |
+200-100 | +325-200 | -325 | ||||
g≤ | 5tPa | |||||||||||
JSF 100.23.10 |
9-11 | 0.30 | 2.10-2.40 | 36 | ¡¡ | ≤3 | 35-50 | balance | 12-25 | High oil immersion rate, high formability | Oilless bearings, PM parts | |
JSF 100.23.18 |
17-20 | 0.30 | 2.10-2.40 | 36 | ¡¡ | ≤3 | 35-50 | balance | 12-25 | |||
JSF 200.23.18 |
17-20 | 0.30 | 2.40-2.60 | 40 | ¡¡ | ¡¡ | +200 | 35-50 | balance | |||
≤5 | ||||||||||||